Blog
Young's Modulus vs Temperature: How Stiffness Changes
Young's modulus usually falls as temperature rises. Learn why, how steels and ceramics behave, and how to measure the curve with impulse excitation.
On this page
Key takeaways
- Young’s modulus of most metals and ceramics decreases as temperature rises; wrought AISI 316L stainless steel goes from 196 GPa at 24 °C to 132 GPa at 800 °C in BAM reference data, a loss of about one third.
- The fall is close to linear in stable, single-phase materials and becomes steep and non-linear near phase transformations or where grain boundaries soften.
- Some materials stiffen on heating: carbon-bonded alumina refractories showed up to 140 % higher Young’s modulus at 1450 °C than at room temperature, because microcracks close.
- Impulse excitation technique (IET) in a furnace gives the full Young’s modulus vs temperature curve from one specimen, on heating and on cooling, together with damping.
- ASTM C1259 (advanced ceramics) and ASTM C1548 (refractories) are written for ambient temperature but state that the method can be used at high temperatures with suitable equipment and a correction for thermal expansion.
Does Young’s modulus change with temperature?
Yes. Young’s modulus is temperature dependent for virtually every engineering material, and for most metals and ceramics it decreases as temperature increases. The size of the effect varies widely between materials: about a third for an austenitic stainless steel between room temperature and 800 °C, with sudden drops wherever the microstructure changes.
That matters well beyond the laboratory. A turbine component, a kiln shelf, a refractory lining or a brake disc works at temperatures where its stiffness is lower than the room-temperature datasheet value. Thermal stresses, natural frequencies, deflections and thermal shock resistance all scale with the modulus at the operating temperature, not at 20 °C.
Why does Young’s modulus decrease as temperature rises?
Young’s modulus reflects how steeply the force between atoms rises when they are pushed apart or together. Because the interatomic potential is asymmetric, heating does two things: atoms vibrate with larger amplitude, and their average spacing grows (thermal expansion). At the larger spacing the restoring force rises less steeply with displacement, so the material needs less stress for the same elastic strain. This is textbook solid-state physics, and it explains the smooth, gradual decrease seen in stable materials.
Two further mechanisms produce the sharper changes engineers often see in practice:
- Phase transformations. When the crystal structure changes, the elastic constants change with it. In AISI 4130 steel, a 2023 IET study in Crystals found that the dynamic Young’s and shear moduli of annealed material decrease linearly up to 650 °C, followed by a sharp decrease between about 650 and 900 °C, together with a strong damping peak, during the transformation from ferrite and cementite to austenite.
- Grain-boundary softening. In their classic 1959 study of refractory materials, Wachtman and Lam found that for most polycrystalline oxides Young’s modulus decreased approximately linearly with temperature until a characteristic temperature range was reached, above which it fell very rapidly and non-linearly. They attributed this to grain-boundary slip. Single-crystal sapphire, which has no grain boundaries, kept decreasing linearly.
Young’s modulus vs temperature for steel: reference data
Steel is one of the most searched cases, and it shows the typical metallic behaviour clearly. The Bundesanstalt für Materialforschung und -prüfung (BAM) published temperature-dependent Young’s and shear modulus data for AISI 316L, Ti-6Al-4V and IN718 as audited reference data (Rehmer et al., Scientific Data, 2023). The measurements were made by the resonance method in vacuum, with dimensions corrected for thermal expansion at each temperature step. The table below is taken from the published dataset for one wrought (hot-rolled, solution-annealed) 316L specimen, St_C_1 (BAM reference data on Zenodo).
| Temperature | Flexural frequency (flat-wise) | Young's modulus E | Shear modulus G | E relative to 24 °C |
|---|---|---|---|---|
| 24 °C | 1528 Hz | 196 GPa | 76 GPa | 100 % |
| 200 °C | 1467 Hz | 180 GPa | 70 GPa | 92 % |
| 400 °C | 1396 Hz | 163 GPa | 62 GPa | 83 % |
| 600 °C | 1326 Hz | 146 GPa | 56 GPa | 74 % |
| 800 °C | 1263 Hz | 132 GPa | 50 GPa | 67 % |
Three points stand out for anyone who uses such data:
- The decrease is large and nearly linear. Between 24 °C and 800 °C this austenitic steel lost about 33 % of its Young’s modulus and about 34 % of its shear modulus, at a fairly constant average rate of about 8 GPa per 100 °C.
- Frequency carries the signal. The flexural resonance frequency fell from 1528 Hz to 1263 Hz. Because Young’s modulus is proportional to the square of the frequency, a 17 % drop in frequency corresponds to a much larger drop in stiffness.
- Thermal expansion must be corrected. The 100.0 mm bar was 101.5 mm long at 800 °C. Using the room-temperature dimensions would overestimate E by roughly 1.5 % at that temperature (our calculation from the dataset), which is a systematic error comparable to the stated measurement uncertainty.
BAM reports a measurement uncertainty of at most 1 % for Young’s modulus at room temperature and 3 % at high temperature. The authors also note that dynamic (adiabatic) moduli are slightly higher than isothermal values, which is worth remembering when comparing resonance data with slow static tests.
How ceramics and refractories behave
Ceramics show a much wider range of behaviour than metals, and the microstructure, not just the chemistry, decides the shape of the curve.
| Material type | Typical Young's modulus vs temperature behaviour | Main cause |
|---|---|---|
| Single-crystal oxides (sapphire) | Linear decrease up to the highest temperature measured | Lattice anharmonicity only |
| Dense polycrystalline oxides (alumina, magnesia) | Near-linear decrease, then a rapid non-linear drop above a material-specific temperature | Grain-boundary slip at high temperature |
| Stabilised zirconia, spinel | Non-linear already at low temperature, rapid drop at high temperature | Material-specific; reported by Wachtman and Lam |
| Carbon-bonded refractories | Increase on heating, strong hysteresis on cooling | Microcracks close on heating and reopen on cooling |
| Steels (for comparison) | Near-linear decrease, sharp drop at phase transformation | Lattice softening, then α to γ transformation |
Sources: Wachtman and Lam, 1959; Journal of the American Ceramic Society, 2013; Crystals, 2023.
The carbon-bonded case is the one that surprises people. In a 2013 study in the Journal of the American Ceramic Society, sintered alumina and carbon-bonded alumina materials with 20 and 30 wt % carbon were measured by impulse excitation from 25 °C to 1450 °C. The Young’s modulus of the carbon-bonded materials increased by up to 140 % at 1450 °C, and after one thermal cycle it was up to 50 % lower at room temperature than before. The authors linked this to the different thermal expansion of alumina grains and graphite flakes: microcracks form during cooling and close again during heating. For materials like these, a heating-and-cooling curve says far more than a single room-temperature value. Our guide to impulse excitation testing for ceramics, glass and refractories covers testing these materials in more detail.
The Wachtman equation for temperature-dependent modulus
A widely used empirical model for Young’s modulus vs temperature is the Wachtman equation. In 1961 Wachtman and co-workers measured several oxides between 77 K and 850 K by a resonance technique and found that the temperature dependence was described very well by a term of the form T·exp(−T₀/T) (Physical Review, 1961). Written out:
E(T) = E₀ − B·T·exp(−T₀/T)
where E₀ is the modulus at absolute zero, T is the absolute temperature in kelvin, and B and T₀ are constants fitted to the data. At high temperature the exponential term approaches 1 and the curve becomes a straight line, which matches the near-linear decrease seen in the steel data above.
Wachtman’s group had no theoretical basis for the formula at first. Anderson later showed that it is equivalent to a bulk-modulus equation derived from the Mie-Grüneisen equation of state, and that it applies to Young’s modulus only when Poisson’s ratio changes little with temperature (Physical Review, 1966).
In practice, the equation is useful for smoothing, interpolating and extrapolating data from a stable material over a moderate range. It cannot predict phase transformations, microcrack closure, grain-boundary softening, sintering or oxidation, which are exactly the effects that cause trouble in service. It describes measured curves; it does not replace them.
How to measure Young’s modulus at high temperature
Impulse excitation technique (IET) is a non-destructive method that determines Young’s modulus, shear modulus and damping from the natural vibration of a specimen after a light mechanical impulse. At high temperature the procedure is the same as at room temperature, carried out in a furnace:
- A bar, rod or disc is placed on supports at the nodal lines of the vibration mode, inside the furnace.
- The furnace follows a programmed heating and cooling cycle, with soak times so the specimen temperature is uniform at each measurement point.
- At each step the excitation system gives the specimen a light impulse, and the acoustic response is recorded and analysed by FFT to find the flexural (and, if needed, torsional) resonance frequency and its damping, the −3 dB bandwidth in Hz.
- Young’s modulus is calculated from the frequency, the mass and the dimensions, with the dimensions corrected for thermal expansion at that temperature.
The standards support this. ASTM C1259 for advanced ceramics covers ambient temperature, but its scope states that the method “can also be performed at cryogenic and high temperatures with suitable equipment modifications and appropriate modifications to the calculations to compensate for thermal expansion” (ASTM C1259). ASTM C1548 for refractories contains equivalent wording. The basic calculations are explained in our guide to ASTM E1876.
Compared with static tests at temperature, the resonance approach has clear practical advantages. One specimen yields the whole curve, so specimen-to-specimen scatter does not blur the trend. Strains are tiny, so the measurement does not damage or creep the specimen. And damping is recorded at every point: a damping peak that coincides with a change in slope of the modulus curve is a strong indicator of a phase transformation or microstructural change, as in the AISI 4130 study.
GrindoSonic offers this capability with the HT1600 high-temperature option, which measures Young’s modulus, shear modulus, natural frequencies and damping in Hz against temperature from room temperature up to 1600 °C, together with a GrindoSonic system such as the GrindoSonic MK7.
Practical tips for reliable high-temperature data
High-temperature IET is straightforward, but a few details decide whether the curve can be trusted:
- Use expansion data for the actual material. The dimensional correction needs the coefficient of thermal expansion over the full range. Where it is unknown, measure it by dilatometry on the same material.
- Allow soak time. BAM used soak times of 10 to 25 minutes at each step. Measuring during a fast ramp introduces temperature gradients and a lag between the thermocouple reading and the specimen temperature.
- Measure on cooling as well as heating. Hysteresis between the two curves reveals microcracking, sintering or irreversible phase changes, and a permanent change at room temperature after the cycle shows damage.
- Watch the atmosphere. Metals and carbon-containing materials oxidise in air at high temperature. BAM measured its alloys in a vacuum furnace; an inert-gas atmosphere is the usual alternative.
- Check the resonance peak, not just the number. A broadening peak, a growing −3 dB bandwidth or a second peak close by indicates that something is happening in the material. Our article on how to read a clean FFT explains what to look for.
For background on the physics behind the measurement, see the fundamentals guide.
What the curve tells a quality or design engineer
A Young’s modulus vs temperature curve is more than an input for finite element models. For a design engineer it gives the stiffness at the real operating temperature, which feeds directly into thermal stress, deflection and natural-frequency calculations. For a materials developer it shows where the microstructure changes: the onset of grain-boundary softening, a phase transformation, or the temperature at which microcracks close. For a refractory or ceramics producer it shows whether a new formulation keeps its stiffness, and whether a thermal cycle leaves permanent damage.
The common thread is that room-temperature values are not enough. A datasheet that gives 196 GPa for an austenitic stainless steel is correct at 24 °C but about 48 % too high at 800 °C, where the measured value is 132 GPa. Measuring the curve on your own material, in its own heat-treatment condition, is the only way to know how it behaves where it actually works.
Frequently Asked Questions
Does Young's modulus change with temperature?
Why does Young's modulus decrease with increasing temperature?
Is there an equation for Young's modulus as a function of temperature?
How do you measure Young's modulus at high temperature?
How much does Young's modulus of steel drop at 600 °C?
Related Posts
Heat treatment changes Young's modulus far less than strength, but not zero. See measured data for steel, titanium and aluminium, and how IET detects it.
Young's Modulus of Cast Iron: Grey, CGI and DuctileYoung's modulus of cast iron ranges from about 69 to 145 GPa for grey iron grades and rises with nodularity. Why it varies and how to measure it reliably.
Damping Properties Testing for Ceramics and Metals: A Step-by-Step GuideA practical step-by-step guide to measuring damping in ceramics and metals with the Impulse Excitation Technique (IET) — from specimen preparation and support placement to signal interpretation and GO/NOGO decisions.
Application notes
Get new IET application notes
Occasional, genuinely useful notes on measuring elastic properties and damping non-destructively. No sales fluff, unsubscribe anytime.
Ready to Get Started?
Contact us to discuss your requirements and see how IET can help.