All Posts

Blog

Young's Modulus of Cast Iron: Grey, CGI and Ductile

Young's modulus of cast iron ranges from about 69 to 145 GPa for grey iron grades and rises with nodularity. Why it varies and how to measure it reliably.

GrindoSonic 11 min read
youngs-modulusmetalsquality-controlnon-destructive-testingcast-iron
On this page

Key takeaways

  • Young’s modulus of cast iron depends mainly on the shape and amount of graphite: handbook values for ASTM A48 grey iron run from about 69 GPa (Class 20) to about 145 GPa (Class 60), against about 210 GPa for steel.
  • Grey iron is not linear-elastic in tension, so its static modulus depends on how it is measured; one study of GJL-150 quotes literature values of 78 to 103 GPa.
  • Within one grey iron family, composition matters: brake disc irons with a eutectic saturation degree of 0.88 to 1.01 measured roughly 100 to 140 GPa, with lower stiffness at higher carbon saturation.
  • Moving from flake to nodular graphite raises modulus. Ultrasonic velocity changes by up to 5 % between 15 % and 100 % nodularity, roughly a 10 % change in modulus.
  • Because resonant frequency follows modulus, a tap test of a few seconds per part can screen every casting for graphite form, which is how IET is used for nodularity control.

What is the Young’s modulus of cast iron?

The Young’s modulus of cast iron is not one number: it ranges from below 70 GPa for low-strength grey iron to values approaching steel for fully nodular ductile iron. The matrix of most cast irons (ferrite, pearlite or a mix) is essentially steel. What changes the stiffness is the graphite, which has very little load-bearing capacity in the form it takes in cast iron and acts largely like a population of voids or cracks.

European standards group cast irons by graphite shape. As summarised in a 2026 paper in Materials by Zych and co-authors, EN 1560 recognises flake graphite iron (EN-GJL-100 to EN-GJL-350), vermicular or compacted graphite iron (EN-GJV-300 to EN-GJV-500) and spheroidal graphite iron (EN-GJS-350-22 to EN-GJS-900-2). Only a small share of off-form graphite is tolerated: up to 5 % in ductile iron and up to 20 % in vermicular iron, where EN 16079 calls for at least 80 % vermicular graphite.

For grey iron, the handbook table reproduced on Wikipedia’s grey iron page gives the tensile modulus per ASTM A48 class:

ASTM A48 classTensile strength (ksi)Tensile modulus (Mpsi)Tensile modulus (GPa, converted)
202210≈ 69
303114≈ 97
405718≈ 124
6062.521≈ 145

The same source explains the trend: the modulus of the grades reflects their graphite content, because graphite has neither strength nor stiffness and the space it occupies behaves like a void. Stronger classes have a lower carbon equivalent and so contain less graphite, which brings them closer to the matrix stiffness.

Grey, compacted graphite and ductile iron compared

The three families differ in stiffness in the same order as their graphite becomes more compact: flake, then vermicular, then spheroidal. Ductile iron is the stiffest, grey iron the most compliant, and compacted graphite iron (CGI) falls between them.

FamilyGraphite formRelative stiffnessTypical reason for variation
Grey iron (EN-GJL)Interconnected flakesLowest; strongly grade-dependentFlake size, length and graphite volume fraction
Compacted graphite iron (EN-GJV)Vermicular, with some nodulesIntermediateShare of vermicular versus nodular graphite
Ductile iron (EN-GJS)Spheroids (nodules)Highest; closer to steelNodularity, nodule count, matrix

The ultrasonic data quoted in US patent 5,714,688, citing Henderson’s work in the Foundry Trade Journal, show the same order: about 170,000 inches per second (≈ 4.3 km/s) for grey iron against about 225,000 inches per second (≈ 5.7 km/s) for ductile iron. The patent also states the underlying rule plainly: the change from flake to nodular graphite is related to an increase in both modulus of elasticity and strength.

Ductile iron grades are often quoted with a narrow modulus range, but that range still moves with nodularity and matrix. For design work, use a value measured on your own grade, section size and heat treatment, not a generic figure from a table.

Why grey iron gives so many different modulus values

Published values for grey iron disagree mostly because grey iron does not have one static modulus. In tension, it is non-linear from the start. A 2021 study in Metals from the Karlsruhe Institute of Technology explains that graphite lamellae act as microcracks even at very small strains and transmit almost no force, while stress peaks build at their sharp tips. Under compression the lamellae are pressed together, carry load, and the iron behaves more like steel. The result is a tension–compression asymmetry with load-dependent Young’s moduli.

Because the stress–strain curve has no clear linear section, ASTM E111 allows a tangent or secant modulus, and the KIT authors note that these give different results depending on the strain at which they are evaluated. Their simulated GJL-150 microstructures gave tensile secant moduli of 106 to 112 GPa, compared with literature values of 78 to 103 GPa for real GJL-150. Their simulations also showed that, under tensile load, both Young’s modulus and yield strength fall as the graphite volume fraction rises from 10 to 12 vol.%; under compression the trend reverses.

Three consequences matter in practice:

  1. A static modulus from a tensile test depends on the evaluation strain, so two laboratories can report different numbers for the same iron.
  2. Tension and compression give different values, which matters for finite element models of parts loaded in bending.
  3. A dynamic measurement subjects the specimen to only minute strains, so the modulus is measured at or near the origin of the stress–strain curve. This avoids most of the evaluation-strain ambiguity and gives a single, repeatable value for comparison between batches.

How composition shifts stiffness within a grade

Even inside one grey iron grade, small changes in carbon and silicon move the modulus. The quantity foundries track is the eutectic saturation degree (SC): the higher it is, the lower the strength and stiffness of the iron.

A 2024 study by Zyska and co-authors in Materials, carried out with a brake disc foundry, tested 180 ventilated discs cast from three pearlitic grey iron grades with SC between 0.88 and 1.01. Ultrasonic measurements on the discs gave an elastic modulus of roughly 100 to 140 GPa, with standard deviations of 2.3 to 4.3 GPa. The grade with the lowest saturation had the highest modulus and strength. The grade with the highest saturation had the lowest.

The same work linked these material differences to the parts themselves. With the optimum composition, the first natural frequency of the smaller disc design (322 mm) ranged from 1001 to 1090 Hz across the grades, and that of the larger design (380 mm) from 724 to 780 Hz. Moving composition from the optimum to the permitted minimum or maximum shifted the natural frequency by several to several dozen hertz. The authors report that the permitted range for the first natural frequency is agreed with each customer and is most often 3 to 5 % of the ordered value. This is why brake disc producers treat modulus and natural frequency as controlled quantities, not as fixed material constants.

Nodularity, resonant frequency and the tap test

Nodularity can be screened through resonant frequency because frequency follows modulus. For a part of fixed geometry and mass, the resonant frequency is proportional to the square root of Young’s modulus divided by density (textbook beam theory). A casting with degraded nodularity is less stiff and therefore rings at a lower frequency than a good casting of the same shape.

The size of the effect is known from ultrasonic work. Henderson found that longitudinal wave velocity can change by as much as 5 % between 15 % and 100 % nodularity, and the patent cited above notes that velocity changes in proportion to the square root of Young’s modulus. A 5 % velocity change therefore corresponds to roughly a 10 % change in modulus at constant density. In Henderson’s data, castings specified at 80 % minimum nodularity needed a minimum velocity of 223,000 inches per second as cast and 217,000 inches per second after heat treatment, which shows that the acceptance limit depends on the process condition as well as the graphite.

Research on cast irons with deliberately mixed graphite forms adds a useful detail. Zych and co-authors found that the dynamic modulus of their ferritic irons varies within wide limits with the average graphite shape index, with the main changes occurring once the shape index falls below 0.6. In practice, a fully nodular iron and a slightly degraded one differ less than a degraded iron and one that has drifted towards vermicular or flake graphite.

GrindoSonic’s own history runs through this application. An appraisal of the original GrindoSonic instrument by the British Cast Iron Research Association (BCIRA) found that its readings on iron test bars with different nodularity and pearlite contents corresponded very well with BCIRA’s forced-vibration sonic test equipment. The report notes that resonant frequency is a satisfactory indication of the form and amount of graphite, that a single test takes a few seconds, and that testing rates of about 500 castings per hour were limited by handling rather than by the measurement.

How to measure Young’s modulus of cast iron with IET

Impulse excitation technique (IET) measures Young’s modulus by tapping a specimen lightly and recording the frequency at which it vibrates. For a machined bar, the flexural resonance frequency, mass and dimensions give the dynamic Young’s modulus; the torsional frequency gives the shear modulus, and the two together give Poisson’s ratio. ASTM E1876 covers this method at ambient temperature; its calculations are valid for materials that are elastic, homogeneous and isotropic, and a sound cast iron test bar, with its graphite finely distributed through the section, is normally treated as such at the scale of the specimen.

A practical sequence for a foundry laboratory:

  1. Machine a rectangular or cylindrical bar from a separately cast or attached test block, with parallel faces and a length of several times its thickness. Weigh it and measure it precisely, since dimensional error feeds directly into the modulus.
  2. Support the bar on its flexural nodal lines, at about 22.4 % of the length from each end, and tap it at the centre with the excitation system. Read the flexural frequency, then repeat for the torsional mode.
  3. Calculate E and G with the ASTM E1876 equations. Record the damping as the −3 dB bandwidth in Hz of the flexural peak, together with the frequency it belongs to. Graphite-rich grey irons and ferritic matrices damp more strongly than low-carbon-equivalent or pearlitic irons, so damping adds information that frequency alone does not give.
  4. For production castings, skip the modulus calculation. ASTM E1876 notes that resonant frequencies alone can be used for quality control and acceptance. Build a frequency window from castings of verified nodularity, then test every part against it.

Our guide on measuring elastic properties gives the full procedures for bars, cylinders and discs, and the article on setting pass/fail thresholds covers how to build an acceptance window from reference parts. The GrindoSonic MK7 covers both tasks: it determines E, G, Poisson’s ratio and damping for bar, disc and cylinder specimens, and with its GO/NOGO quality-control software it applies tolerance bands on frequency and damping for pass/fail screening of castings.

Using modulus data in design and quality control

Treat the modulus of cast iron as a process output that needs measuring, not a constant to look up. The same nominal grade can vary by tens of GPa with carbon saturation, section size, cooling rate and inoculation, and those variations show up directly in stiffness, natural frequency and noise behaviour.

For design engineers, this means asking suppliers for measured dynamic modulus values on the actual grade and section, and using the matching value in modal and stiffness calculations. For foundries, it means a short loop: measure modulus or frequency on test bars, link it to metallography and tensile data once, then use the frequency alone as a fast, non-destructive check on every casting. Parts outside the window go to the metallurgical laboratory. Parts inside it ship with a recorded measurement.

Frequently Asked Questions

What is the Young's modulus of cast iron?
There is no single value. Handbook data for ASTM A48 grey iron run from about 69 GPa for Class 20 to about 145 GPa for Class 60. Compacted graphite iron sits higher, and ductile iron is the stiffest family, though still below steel at around 210 GPa. The graphite shape and amount set the value, so grade-specific measured data are needed for design.
Why is the elastic modulus of grey cast iron lower than steel?
Grey iron has a steel-like matrix interrupted by graphite flakes. Under tension the flakes carry almost no load and behave like internal cracks, so the effective stiffness of the casting drops. The more graphite and the larger and longer the flakes, the lower the modulus. Ductile iron, with graphite in compact nodules, loses far less stiffness.
Does nodularity affect Young's modulus?
Yes. Moving from flake to nodular graphite raises both modulus and strength, which is why ultrasonic velocity and resonant frequency are used as guides to nodularity. Henderson's ultrasonic data showed longitudinal sound velocity changing by up to 5 % between 15 % and 100 % nodularity, which corresponds to roughly a 10 % change in modulus.
Why do published values for grey iron modulus disagree?
Grey iron is not linear-elastic in tension, so a static tensile test gives a secant or tangent modulus that depends on the strain at which it is evaluated. Tension and compression also give different values. A dynamic measurement such as impulse excitation applies only minute strains, so it measures the modulus at or near the origin of the stress–strain curve and gives one repeatable number for comparison.
How do foundries check nodularity without cutting the casting?
They measure a property that depends on modulus: ultrasonic velocity or resonant frequency. A casting is tapped, its resonant frequency is compared with limits set from castings of known nodularity, and parts outside the window are sent for metallography. A single test takes seconds, so every casting can be checked.

Ready to Get Started?

Contact us to discuss your requirements and see how IET can help.